In the present study, the structural and creep resistance properties of S9Z1 alloys with Cu-addition in concentrations (0.1 and 0.3% Wt.) have been investigated using x-ray diffractions (XRD) and Creep testing machine respectively. The three samples were prepared from high purity 99.99% by melting technique in the Pyrex tubs with CaCl2 to invaded the oxidation. The obtained samples were rolled drawn (cold rolling) into two groups. The first group was as wires for the creep resistance testing. The second group was as small sheets for structural investigations. Patterns of XRD showed that the S9Z1 alloy was primarily composed of two phases; a body centered tetragonal β-Sn matrix phase, and a secondary phase of hexagonal Zn. while with addition Cu (0.1 and 0.3% Wt.) to S9Z1 Alloys the results showed new peaks in the ternary compositions, such as Cu6Sn5, Cu5Zn8, phases respectively. The average of particle size (D) of β-Sn matrix was decreased with increasing Cu -adding, whereas the dislocation density (δ) increased with increasing addition. Creep properties of S9Z1, S9Z2 and 3 Alloys were examined at different temperatures (25, 40 and 80°C) under two constant loads (σ= 18.7 and 24.94 MPa). The creep behaviors of ternary alloys were higher than the S9Z1 alloys with all different temperatures under two constant loads. Also, the S9Z3 alloy with all different temperatures and two loads exhibited greatest creep resistance, due to the refinement structure and formation of new IMCs. Values of stress exponent (n) were found to be in the range of 1 to 10.55, for all S9Z2 and 3 alloys respectively. Values of activation energy (Q) of alloys were found to be in the range of 36.48 to 37.49 kJ/mol, for σ = 18.7 Mpa and 27 to 34.8 kJ/mol for σ = 24.94 Mpa for the S9Z1 alloys with Cu addition respectively. At room temperature (25°C), the electrical conductivity of the samples was calculated, and its values increased with Cu additions.
Published in | International Journal of Materials Science and Applications (Volume 13, Issue 4) |
DOI | 10.11648/j.ijmsa.20241304.11 |
Page(s) | 61-70 |
Creative Commons |
This is an Open Access article, distributed under the terms of the Creative Commons Attribution 4.0 International License (http://creativecommons.org/licenses/by/4.0/), which permits unrestricted use, distribution and reproduction in any medium or format, provided the original work is properly cited. |
Copyright |
Copyright © The Author(s), 2024. Published by Science Publishing Group |
S9Z-xCu, Lead-Free Alloy, Phases, Cu-Additions, Creep Resistance, Structural Properties, Electrical Conductivity
S. No. | Alloys | Sn | Zn | Cu |
---|---|---|---|---|
1 | S9Z1 | 91 | 9 | 0 |
2 | S9Z2 | 90.9 | 9 | 0.1 |
3 | S9Z3 | 90.7 | 9 | 0.3 |
S. wt% | Phases | peaks | Crystal system | (JCPDS-ICDD)Re. |
---|---|---|---|---|
S9Z1 | β-Sn | 9 | Body centered tetragonal | PDF#04-0673 |
Zn | 5 | Hexagonal | PDF#04-0831 | |
S9Z2 | β-Sn | 9 | Body centered tetragonal | PDF#04-0673 |
Zn | 1 | Hexagonal | PDF#04-0831 | |
Cu6Sn5 | 3 | Monoclinic | PDF#45-1488 | |
Cu5Zn8 | 1 | Cubic | PDF#25-1228 | |
S9Z3 | β-Sn | 9 | Body centered tetragonal | PDF#04-0673 |
Zn | 1 | Hexagonal | PDF#04-0831 | |
Cu6Sn5 | 1 | Monoclinic | PDF#45-1488 | |
Cu5Zn8 | 3 | Cubic | PDF#25-1228 |
S. in wt.% | D β-Sn (nm) | D Zn (nm) | D Cu5Zn8 (nm) | D Cu6Sn5 (nm) | (ƹ) x10-3 of β-Sn phase | c/a of β-Sn phase | V (Å)3 of β-Sn phase | δ (nm) (-2) *10-3 of β-Sn phase |
---|---|---|---|---|---|---|---|---|
S9Z1 | 23.6 | 16.4 | - | - | 1.2 | 0.542 | 109.14 | 179 |
S9Z2 | 16.5 | 16.1 | 3.8 | 9.7 | 1.8 | 0.547 | 109.7 | 367 |
S9Z3 | 16.4 | 13.77 | 14.7 | 3.5 | 1.6 | 0.55 | 110.7 | 374 |
S. | EL.% | |||||
---|---|---|---|---|---|---|
18.7 MPa | 24.94 MPa | |||||
Tem. | 25°C | 40°C | 80°C | 25°C | 40°C | 80°C |
S9Z1 | 4.92 | 7.45 | 16..74 | 11.38 | 26.39 | 16.55 |
S9Z2 | 3.94 | 6.64 | 14.1 | 5.04 | 27.62 | 15.26 |
S9Z3 | 2.83 | 3.26 | 5.72 | 3.07 | 8 | 7.26 |
S. in%wt. | Q (KJ/mol) | Av. Q (KJ/mol) | |
---|---|---|---|
18.7 MPa | 24.94 MPa | ||
S9Z1 | 36.48 | 27 | 31.74 |
S9Z2 | 37.97 | 33.98 | 35.98 |
S9Z3 | 37.49 | 34.8 | 36.15 |
S. in Wt.% | (Ω-Cm) * 10-3 | (Ω-Cm)–1 |
---|---|---|
S9Z1 | 1.83 | 546.45 |
S9Z2 | 1.13 | 884.96 |
S9Z3 | 1.12 | 892.88 |
°C | Temperature Percentage " Celsius" |
β | Rigid Solution |
Sn | Tin |
Zn | Zinc |
Cu | Copper |
XRD | X-Ray Diffraction |
FWHM | Full Width at Half Maximum |
IMC | Intermetallic Compound |
MPa | Mega Pascal |
RT | Room Temperature |
D | Particle Size |
𝛿 | Dislocation Density |
JCPDS-ICDD | Joint Committee on Powder Diffraction Standards at the International Center for Diffraction Data |
[1] | Sharif, A., Y. C. J. J. o. a. Chan, and compounds, Investigation of interfacial reactions between Sn–Zn solder with electrolytic Ni and electroless Ni (P) metallization. 2007. 440(1-2): p. 117-121. |
[2] |
Billah, M. M., K. M. J. A. M. Shorowordi, and Materials, Effect of micron size Ni particle addition on microstructure, thermal and mechanical properties of Sn-9Zn lead-free solder alloy. 2012. 229: p. 271-275.
http://dx.doi.org/10.4028/www.scientific.net/AMM.229-231.271 |
[3] | Olufemi, A. C., et al., Potential health risks of lead exposure from early life through later life: implications for public health education. 2022. 19(23): p. 16006. |
[4] | Wang, H., et al., Effect of lead exposure from electronic waste on haemoglobin synthesis in children. 2021. 94: p. 911-918. |
[5] | Raabe, D. J. C. r., The materials science behind sustainable metals and alloys. 2023. 123(5): p. 2436-2608. |
[6] | Mohamed, H., et al., Evaluation of the microstructure, thermal, and mechanical characteristics of Sn-9Zn reinforced with Ni and ZrO2 nanoparticles via vacuum melting process. 2023. 98(10): p. 105912. |
[7] | El-Daly, A., et al., Thermal and mechanical properties of Sn–Zn–Bi lead-free solder alloys. 2009. 484(1-2): p. 134-142. |
[8] | Negm, S. E. A., A. A. Moghny, and S. I. J. R. i. M. Ahmad, Investigation of thermal and mechanical properties of Sn-Zn and Sn-Zn-Bi near-eutectic solder alloys. 2022. 15: p. 100316. |
[9] | Lin, P., et al., Effect mechanism of Ag and Bi elements on the corrosion process in Sn–9Zn–1Ag and Sn–9Zn–3Bi solders. 2019. 6(11): p. 1165a2. |
[10] | Zhang, L., et al., Development of Sn–Zn lead-free solders bearing alloying elements. 2010. 21: p. 1-15. |
[11] | Liu, S., et al., Present status of Sn–Zn lead-free solders bearing alloying elements. 2015. 26: p. 4389-4411. |
[12] | Gerhátová, Ž., et al., Microstructure and corrosion behavior of Sn–Zn alloys. 2022. 15(20): p. 7210. |
[13] | El-Daly, A., Y. Swilem, and A. Hammad, Creep properties of Sn–Sb based lead-free solder alloys. Journal of Alloys and Compounds, 2009. 471(1-2): p. 98-104. |
[14] | Cheng, S., C.-M. Huang, and M. J. M. R. Pecht, A review of lead-free solders for electronics applications. 2017. 75: p. 77-95. |
[15] | Salem, M. Y. J. A. J. o. N. S. and Applications, Effect of small addition Indium on transient and steady-state creep characteristics, microstructure and properties of Sn-9Zn lead-free solders. 2018. 51(3): p. 69-86. |
[16] | Shrestha, T., et al., Creep deformation behavior of Sn–Zn solder alloys. 2014. 49: p. 2127-2135. |
[17] | Chen, K.-I., et al., Effects of small additions of Ag, Al, and Ga on the structure and properties of the Sn–9Zn eutectic alloy. 2006. 416(1-2): p. 98-105. |
[18] | Yu, D., et al., Investigation of interfacial microstructure and wetting property of newly developed Sn–Zn–Cu solders with Cu substrate. 2004. 385(1-2): p. 119-125. |
[19] | Al-Salmi, M., et al., Silver (Ag) Improvements on The Structural, Creep Resistance and Electrical Conductivity Properties of Eutectic Sn-9Zn Alloys. 2020. 2(3): p. 142-155. |
[20] | El-Daly, A., A. J. J. o. A. Hammad, and Compounds, Elastic properties and thermal behavior of Sn–Zn based lead-free solder alloys. 2010. 505(2): p. 793-800. |
[21] | El-Daly, A. and A. Hammad, Effects of small addition of Ag and/or Cu on the microstructure and properties of Sn–9Zn lead-free solders. Materials Science and Engineering: A, 2010. 527(20): p. 5212-5219. |
[22] | Williamson, G. and W. J. A. m. Hall, X-ray line broadening from filed aluminium and wolfram. 1953. 1(1): p. 22-31. |
[23] | Tanaka, M., et al. Improvement in drop shock reliability of Sn-1.2 Ag-0.5 Cu BGA interconnects by Ni addition. in 56th Electronic Components and Technology Conference 2006. 2006. IEEE. |
[24] | D'Souza, R. C., et al., Comparative study on tensile creep behavior of SN-9ZN, SN-0.7 CU and SN-49ZN-1CU solders. 2013. |
[25] | Wu, C. M. L and Huang, M, L.. Creep behavior of eutectic Sn-Cu Lead-Free Solder Alloys. Journal of Electronic Materials. 2002. |
[26] | El-Daly, A., et al., The effect of undercooling on the microstructure and tensile properties of hypoeutectic Sn–6.5 Zn–xCu Pb-free solders. Materials & Design, 2015. 80: p. 152-162. |
[27] | El-Daly, A., et al., Design of lead-free candidate alloys for low-temperature soldering applications based on the hypoeutectic Sn–6.5 Zn alloy. Materials & Design (1980-2015), 2014. 56: p. 594-603. |
[28] | Chen, Z., Y. Shi, and Z. Xia, Constitutive relations on creep for SnAgCuRE lead-free solder joints. Journal of electronic materials, 2004. 33(9): p. 964-971. |
[29] | Glazer, J., Metallurgy of low temperature Pb-free solders for electronic assembly. International Materials Reviews, 1995. 40(2): p. 65-93. |
[30] | Callister, W. D., et al., Materials science and engineering: an introduction. Vol. 7. 2007: John wiley & sons New York. |
[31] | La Barre, K. A., The Art and Science of Classification: Phyllis Allen Richmond, 1921-1997. 2004. |
APA Style
Ali, G. N., Al-Salmi, M. S. N. (2024). Influence of Temperature on Creep Resistance, Structural and Electrical Characteristics of S9Z1 Eutectic Alloys. International Journal of Materials Science and Applications, 13(4), 61-70. https://doi.org/10.11648/j.ijmsa.20241304.11
ACS Style
Ali, G. N.; Al-Salmi, M. S. N. Influence of Temperature on Creep Resistance, Structural and Electrical Characteristics of S9Z1 Eutectic Alloys. Int. J. Mater. Sci. Appl. 2024, 13(4), 61-70. doi: 10.11648/j.ijmsa.20241304.11
AMA Style
Ali GN, Al-Salmi MSN. Influence of Temperature on Creep Resistance, Structural and Electrical Characteristics of S9Z1 Eutectic Alloys. Int J Mater Sci Appl. 2024;13(4):61-70. doi: 10.11648/j.ijmsa.20241304.11
@article{10.11648/j.ijmsa.20241304.11, author = {Gobran Naji Ali and Mohammed Saleh Nasser Al-Salmi}, title = {Influence of Temperature on Creep Resistance, Structural and Electrical Characteristics of S9Z1 Eutectic Alloys }, journal = {International Journal of Materials Science and Applications}, volume = {13}, number = {4}, pages = {61-70}, doi = {10.11648/j.ijmsa.20241304.11}, url = {https://doi.org/10.11648/j.ijmsa.20241304.11}, eprint = {https://article.sciencepublishinggroup.com/pdf/10.11648.j.ijmsa.20241304.11}, abstract = {In the present study, the structural and creep resistance properties of S9Z1 alloys with Cu-addition in concentrations (0.1 and 0.3% Wt.) have been investigated using x-ray diffractions (XRD) and Creep testing machine respectively. The three samples were prepared from high purity 99.99% by melting technique in the Pyrex tubs with CaCl2 to invaded the oxidation. The obtained samples were rolled drawn (cold rolling) into two groups. The first group was as wires for the creep resistance testing. The second group was as small sheets for structural investigations. Patterns of XRD showed that the S9Z1 alloy was primarily composed of two phases; a body centered tetragonal β-Sn matrix phase, and a secondary phase of hexagonal Zn. while with addition Cu (0.1 and 0.3% Wt.) to S9Z1 Alloys the results showed new peaks in the ternary compositions, such as Cu6Sn5, Cu5Zn8, phases respectively. The average of particle size (D) of β-Sn matrix was decreased with increasing Cu -adding, whereas the dislocation density (δ) increased with increasing addition. Creep properties of S9Z1, S9Z2 and 3 Alloys were examined at different temperatures (25, 40 and 80°C) under two constant loads (σ= 18.7 and 24.94 MPa). The creep behaviors of ternary alloys were higher than the S9Z1 alloys with all different temperatures under two constant loads. Also, the S9Z3 alloy with all different temperatures and two loads exhibited greatest creep resistance, due to the refinement structure and formation of new IMCs. Values of stress exponent (n) were found to be in the range of 1 to 10.55, for all S9Z2 and 3 alloys respectively. Values of activation energy (Q) of alloys were found to be in the range of 36.48 to 37.49 kJ/mol, for σ = 18.7 Mpa and 27 to 34.8 kJ/mol for σ = 24.94 Mpa for the S9Z1 alloys with Cu addition respectively. At room temperature (25°C), the electrical conductivity of the samples was calculated, and its values increased with Cu additions. }, year = {2024} }
TY - JOUR T1 - Influence of Temperature on Creep Resistance, Structural and Electrical Characteristics of S9Z1 Eutectic Alloys AU - Gobran Naji Ali AU - Mohammed Saleh Nasser Al-Salmi Y1 - 2024/08/15 PY - 2024 N1 - https://doi.org/10.11648/j.ijmsa.20241304.11 DO - 10.11648/j.ijmsa.20241304.11 T2 - International Journal of Materials Science and Applications JF - International Journal of Materials Science and Applications JO - International Journal of Materials Science and Applications SP - 61 EP - 70 PB - Science Publishing Group SN - 2327-2643 UR - https://doi.org/10.11648/j.ijmsa.20241304.11 AB - In the present study, the structural and creep resistance properties of S9Z1 alloys with Cu-addition in concentrations (0.1 and 0.3% Wt.) have been investigated using x-ray diffractions (XRD) and Creep testing machine respectively. The three samples were prepared from high purity 99.99% by melting technique in the Pyrex tubs with CaCl2 to invaded the oxidation. The obtained samples were rolled drawn (cold rolling) into two groups. The first group was as wires for the creep resistance testing. The second group was as small sheets for structural investigations. Patterns of XRD showed that the S9Z1 alloy was primarily composed of two phases; a body centered tetragonal β-Sn matrix phase, and a secondary phase of hexagonal Zn. while with addition Cu (0.1 and 0.3% Wt.) to S9Z1 Alloys the results showed new peaks in the ternary compositions, such as Cu6Sn5, Cu5Zn8, phases respectively. The average of particle size (D) of β-Sn matrix was decreased with increasing Cu -adding, whereas the dislocation density (δ) increased with increasing addition. Creep properties of S9Z1, S9Z2 and 3 Alloys were examined at different temperatures (25, 40 and 80°C) under two constant loads (σ= 18.7 and 24.94 MPa). The creep behaviors of ternary alloys were higher than the S9Z1 alloys with all different temperatures under two constant loads. Also, the S9Z3 alloy with all different temperatures and two loads exhibited greatest creep resistance, due to the refinement structure and formation of new IMCs. Values of stress exponent (n) were found to be in the range of 1 to 10.55, for all S9Z2 and 3 alloys respectively. Values of activation energy (Q) of alloys were found to be in the range of 36.48 to 37.49 kJ/mol, for σ = 18.7 Mpa and 27 to 34.8 kJ/mol for σ = 24.94 Mpa for the S9Z1 alloys with Cu addition respectively. At room temperature (25°C), the electrical conductivity of the samples was calculated, and its values increased with Cu additions. VL - 13 IS - 4 ER -